Are there any "proper" welders on here that might know the answer to the following question please or at least offer some advice ?

Bit of history first, my kids bought me a TIG welder for my birthday at the end of last month so I've been having a go over the past couple of weeks. It's an ESAB Buddy 160 unit & I'm using pure argon gas. Tungsten is a "grey" one & cup size is No.8, (because that's what the kit came with !!). I have the tungsten protruding about 7/16" & gas flow is around 10 litres per minute. I have varied the tip "stick-out" a bit & gas flow together with the current, but it still happens. Not all the time, but enough to be annoying me !
The last time I ever tried any welding was gas welding in the late seventies, early eighties as an apprentice & obviously equipment has move on a lot since then, but I would say gas & TIG welding, technique wise, were very similar.
At the end of some welds I quite often get little holes appear at the end of a weld. It mainly only seems to happen at the end of welds, (although it does happen occasionally in a weld line if the tungsten touches the pool for example). If you look at the pictures below you will see what I mean.
DSCN3850.JPG

DSCN3851.JPG

DSCN3852.JPG


I appreciate there could well be & most likely is, many variables that "could" cause this, but I'm hoping someone in the know might be able to say or suggest what I should look at, say "yes, that commonly happens because of ........ " if you know what I mean.
That way I could hopefully address this particular issue.

I know & don't expect to become a master welder, but I'd like to get better than I am so that as I'm building my current project I could at least tack brackets, etc in place before I get a proper welder to do a proper job (y)
Obviously it would be great to become a dab hand at welding & produce amazing welding beads, but I am realistic enough to know that takes years & years of practice.
 
Last edited:
You don't, you "stitch cast iron" as I'm sure you know full well !!:ROFLMAO::ROFLMAO:;)
I'd never seen that process, but I just watched a couple of videos.. fascinating...
It looks like you can weld Cast, but you really need special rods....
I've got to weld a cast foot back on a log burner.
 
When you say "downslope time" is that the adjustment you make that once you release the torch button that alters the time the arc seems to remain before extinguishing ?

I have that set low at the moment, position 1, which I assume is the shortest time. I tried it at around 6 or 7, but that seemed to be too long & kept the arc going which melted through the metal I was prasticing on. It seemed better when the arc stopped as soon as I released the torch button.

Are you saying by having this set low that it extinguishes the arc too quickly & that is what might cause the holes ?

I'll try dropping the gas flow as you suggest & increasing the slope down time the next time I have a practice & see what difference that makes. Thank you (y)
 
I'd never seen that process, but I just watched a couple of videos.. fascinating...
It looks like you can weld Cast, but you really need special rods....
I've got to weld a cast foot back on a log burner.
Sorry, I though you were taking the mickey out of my project build !!😂 It being a H****y type thing !

From what I understand you can TIG cast iron, but like you say you need specialist filler rods & you really need to pre-heat the area too.
 
Had a very old woodworking machine welded years ago from what I remember he nearly had the cast glowing before welding it?
 
Just had a quick play & adjusted the gas flow down to 8 & turned the slope down up to No.3 & it has made a difference. I'll have a proper play tomorrow & report back.

Also, noticed I had a bit of a gas leak on the pipe to the torch, but after I'd tightened the connection it still had the problem with the holes at the end of some welds.
 
when you finish at the end of the run, do you keep the torch over the last piece of weld to keep the gas blowing at it....cooling and keeping it clean?
 
I'd never seen that process, but I just watched a couple of videos.. fascinating...
It looks like you can weld Cast, but you really need special rods....
I've got to weld a cast foot back on a log burner.
For a foot on a log burner I'd braze it or drill, tap and bolt
 
when you finish at the end of the run, do you keep the torch over the last piece of weld to keep the gas blowing at it....cooling and keeping it clean?
Yes I do, it has a pre-set post gas timer so the higher the slope-down time the longer the post gas time.
 
It’s basically perrosity mte.. The holes are being caused by a chemical reaction due to a dirty workpiece.. For Tig Welding you MUST be ultra clean with everything..
Your workpiece must be really clean eg down to bare metal and then wiped thoroughly with Acetone ( i use nail varnish remover ) your electrode must be clean and sharpened to a fine point if you contaminate it by touching the electrode into the welding puddle stop, and re sharpen it..
Basically your creating a molten puddle which is more like a mini volcano with explosions going on ( contaminants ) where you need a pure clean uncontaminated molten pool ...
Gas at 10 is good, for steel use a red tip tungsten.. Pre gas if you have that option lays a protective shield of gas to protect the tungsten electrode from burning away basically, 2 seconds is a good start. Post flow is equally important as it provides gas flow over the weld and tungsten electrode which again protects after the arc from the electrode has stopped 3 secs is a good setting here..
Slope up and down if you have it brings the Amps in progressively and Slope down does the opposite it slowly ends the current when you take you finger off the trigger protecting your workpiece from too much heat at the end of your run, eg preventing you from burning a hole through at your finish..

Arc welding and stick welding are totally different to Tig.. Tig is neat, fussy welding..
Stick and Mig etc are much easier, less fussy, more agricultural than tig..

Hope that helps, but your issue from the beads i see in your picture is a lack of cleanness prior to welding, contamination..

X
 
For Tig Welding you MUST be ultra clean with everything..
+1 million....

Invest in stainless steel wire brushes and only use them for cleaning aluminium.

I use pcb contact cleaner (Isopropyl Alcohol, RS PRO 500 ml Tin Isopropyl Alcohol (IPA) for PCBs | RS Components) for cleaning down. Don't use brake cleaner, it leaves an oily residue.

Use clean cloth rags. Don't use paper towel as it snags on sharp edges and leaves contamination.

Do not mix and match tools between steel and aluminium working, all it takes is a fleck of steel on a file to be dragged into aluminium and the weld is contaminated, same with hammers, saws, snips etc.
 
It’s basically perrosity mte.. The holes are being caused by a chemical reaction due to a dirty workpiece.. For Tig Welding you MUST be ultra clean with everything..
Your workpiece must be really clean eg down to bare metal and then wiped thoroughly with Acetone ( i use nail varnish remover ) your electrode must be clean and sharpened to a fine point if you contaminate it by touching the electrode into the welding puddle stop, and re sharpen it..
Basically your creating a molten puddle which is more like a mini volcano with explosions going on ( contaminants ) where you need a pure clean uncontaminated molten pool ...
Gas at 10 is good, for steel use a red tip tungsten.. Pre gas if you have that option lays a protective shield of gas to protect the tungsten electrode from burning away basically, 2 seconds is a good start. Post flow is equally important as it provides gas flow over the weld and tungsten electrode which again protects after the arc from the electrode has stopped 3 secs is a good setting here..
Slope up and down if you have it brings the Amps in progressively and Slope down does the opposite it slowly ends the current when you take you finger off the trigger protecting your workpiece from too much heat at the end of your run, eg preventing you from burning a hole through at your finish..

Arc welding and stick welding are totally different to Tig.. Tig is neat, fussy welding..
Stick and Mig etc are much easier, less fussy, more agricultural than tig..

Hope that helps, but your issue from the beads i see in your picture is a lack of cleanness prior to welding, contamination..

X
+1 million....

Invest in stainless steel wire brushes and only use them for cleaning aluminium.

I use pcb contact cleaner (Isopropyl Alcohol, RS PRO 500 ml Tin Isopropyl Alcohol (IPA) for PCBs | RS Components) for cleaning down. Don't use brake cleaner, it leaves an oily residue.

Use clean cloth rags. Don't use paper towel as it snags on sharp edges and leaves contamination.

Do not mix and match tools between steel and aluminium working, all it takes is a fleck of steel on a file to be dragged into aluminium and the weld is contaminated, same with hammers, saws, snips etc.
Thanks guys, you help & advice is taken on-board, much appreciated.
I'll have another crack at it later on today, got to do some revising first for an upcoming exam !
 
it also looks like your cold welding, eg your filler rod is melting before it reaches the pool and dripping in..

Poss your torch angle is too shallow eg 45 degrees instead of only 15 degrees from vertical,

Sharp clean electrode, stick out 2-3 mill max, torch angle 15 degrees from upright, Filler rod feed into the FRONT of the pool at a 90 degree angel to the torch so torch and filler rod are at 90 degrees to each other..
Argon on 10.. 1.6 mm electrode and filler rod if you have them.

CLEAN everything especially the workpiece and wipe thoroughly with acetone or wife’s nail varnish remover..

Get in real close with you eyes, ( one eye in my case ) tilt your head with the torch angle and get as close as poss .. Strike up the arc and wait till a molten pool occurs then dab the rod into the front of the pool and move torch forward and do the same again.. Dab the rod and move, dab and move dab and more.. get a nice rhythm going and if you touch the electrode down etc stop and re sharpen it then go again ..

One of best tips is make sure your comfortable .. Get the weight of the torch’s lead off your arm which will make your hand steadier.. I hang my lead on a hook above me so i’ve no weight on my wrist etc..

hope this helps ..

Join the Mig welding forum .co.uk

Great tips and help on there for all even beginners from top welders..

X
 
I'm a recent convert to TIG, having used MIG for years and having done some Gas welding years ago.
I wanted to weld Ali at home. so recently brought an AC/DC R-Tech but haven't had much of a chance to try it yet.

I was however lucky enough to get myself on a one day course back in March just before the world got turned on it's head.
Natalie who runs these courses is a Genius COURSES | theironlady, and a great teacher.
She demonstrated the flexibility of TIG by welding her initials in Copper on a stainless sheet using a piece of cut up copper pipe as filler rod!
My MIG welding improved and I've got a good head start with TIG.
I was getting really good TIG welds in Ali and Stainless by the end of a really fun day.

I understand she's a long way from you, but I find that sort of course on the Craftcourses website Creative, craft and artisan courses and workshops where you can chose what you want to learn and where.
I'm sure once we are a bit more free to travel a one day course would be of great benefit.

Nasher.
 
One of the problems for us novices particularly welding alloy is not having a foot pedal to reduce the amperage as the alloy soaks up the heat so quickly .
 
Thanks Noods, obviously I have a few common issues as beginners do. I know I keep holding the torch at too steep an angle, i.e. 45+ degrees to the work piece & when I concentrate to rectify that I forget about the filler rod !! When I do get my cordination right I get what I call a half descent weld !:ROFLMAO: Just need practice & lots of it !!

I'm using the stuff that came in the kit at the moment so that is a grey tungsten, 2.4mm diameter, No.8 cup & 1.6mm filler rod. I've got the flow rate set at 10 litres/minute now.
I will get hold of some red tungstens as has been suggested & give them a try.
I was also going to get some smaller cup size, maybe a No.5 in the hope that it might make seeing the pool easier ?
I have now increased the slope-down time too, which has also made an improvement as too has cleaning the weld area prior to welding. I've had very little if any holes today so things are going the right way.

Initially I was struggling to see the pool because of the size of the cup & the amount of stickout I had. After looking on various YouTube videos for TIG welding they seem to suggest you should have around 1/16" of an inch stickout times the size of your cup so for my No.8 cup that meant around 1/2" of stickout. I have to say that made it much easier to see the pool & dab in the filler rod.
These videos also suggested the flow rate should be double what the cup size is, but that was in CFH so I had to convert that to Litres/minute, but as a rough guide Ltrs/minute seems to be about half what the CFH figure is, (unless I have got that wrong) but it does seem to tally up with previous suggestions for flow rates.
 
One of the problems for us novices particularly welding alloy is not having a foot pedal to reduce the amperage as the alloy soaks up the heat so quickly .
You are right there Birdie, I have noticed a foot pedal makes things a lot easier. My torch has the button on it & trying to hold the torch comfortably & operate the button is much harder than when I had a go on my mates foot operated TIG. You concentrate on the button, then forget about the angle you are holding your torch, then get the torch angle right & forget about the filler rod ! It's a vicious circle at the moment :ROFLMAO:
By rights women should make brilliant welders because they can multi-task :unsure:

I will try to go on a course at some point, my mate did this when he started & it is obviously the best way to start, but covid & the fact that when I'm working it is always away from home it doesn't make it that easy !!
In the meantime I'll practice in my garage & get help like all your advice when I'm struggling.

My machine is only DC so I won't be doing any alloy welding. I really only wanted/intended to weld bits to the bobber that I am building. After the first one I built it became a bit of a pain to take the bit & frame to my mate to get him or one of his welders to do the necessary. I thought it would be much better if I could at least tack the bracket or whatever in place & then just get him to final weld it for me. That way I didn't need to align/set-up/clamp everthing in place again while at my mates, before he could tack, then weld it in place.

Obviously as I get good at tacking things I'll want to get good at welding so like alot of things in life you are always striving to get better at something.
 
For those without a foot pedal these are standard settings for Mild and Stainless steel v the various joints..

I learnt without a pedal and although i have one i offer don’t use it tbh..

i would tend to set the Amps a little low to start and if you don’t get a nice fluid puddle that the angle of your torch/electrode can easily push along just increase it by 5 amps a time until you do..

A tight arc is the main issue when learning..

you need to be comfortable and have a free run for your torch to pass along its path without snags etc.. When you have this you need to get the arc ( tip of the electrode) down to 1-1.5mm from the puddle and be consistent with it..
Get your torch hand comfortable, if need be rest it on something to make it comfortable etc, this trust me makes such a difference..

Get a really good fit up if doing joints, really tight makes it so much easier.. The bigger the gap the harder it is...

If your struggling, try doing the above but without using filler rod.. Just run beads without filler on clean flat steel plate, then do the same and join two flat pieces together without filler rod, ( no gap between the two bits though) clamp the bits of steel down if you can also, stops it warping and moving around on your bench..

X


2DF1AADC-DB60-4DEB-8D7A-127BC9387F00.webp


330AE3BD-6273-4039-85AD-EFF80944F9F1.webp
 
Thanks Noods, obviously I have a few common issues as beginners do. I know I keep holding the torch at too steep an angle, i.e. 45+ degrees to the work piece & when I concentrate to rectify that I forget about the filler rod !! When I do get my cordination right I get what I call a half descent weld !:ROFLMAO: Just need practice & lots of it !!

I'm using the stuff that came in the kit at the moment so that is a grey tungsten, 2.4mm diameter, No.8 cup & 1.6mm filler rod. I've got the flow rate set at 10 litres/minute now.
I will get hold of some red tungstens as has been suggested & give them a try.
I was also going to get some smaller cup size, maybe a No.5 in the hope that it might make seeing the pool easier ?
I have now increased the slope-down time too, which has also made an improvement as too has cleaning the weld area prior to welding. I've had very little if any holes today so things are going the right way.

Initially I was struggling to see the pool because of the size of the cup & the amount of stickout I had. After looking on various YouTube videos for TIG welding they seem to suggest you should have around 1/16" of an inch stickout times the size of your cup so for my No.8 cup that meant around 1/2" of stickout. I have to say that made it much easier to see the pool & dab in the filler rod.
These videos also suggested the flow rate should be double what the cup size is, but that was in CFH so I had to convert that to Litres/minute, but as a rough guide Ltrs/minute seems to be about half what the CFH figure is, (unless I have got that wrong) but it does seem to tally up with previous suggestions for flow rates.
Number 8 cup would normally have stick out at approx 7 mm.. only longer if your trying to weld an angled piece.. The more stick out you have the more gas you will need to protect the pool and the electrode.. General rule is the shorter the better stick out wise, just enough to be able to get a tight 1-1.5mm arc... A Big stick out means the cup is a long way away from the puddle and therefore your shielding gas is not getting to where it needs to be eg at the puddle and protecting the tungsten tip..

X
 
You are right there Birdie, I have noticed a foot pedal makes things a lot easier. My torch has the button on it & trying to hold the torch comfortably & operate the button is much harder than when I had a go on my mates foot operated TIG. You concentrate on the button, then forget about the angle you are holding your torch, then get the torch angle right & forget about the filler rod ! It's a vicious circle at the moment :ROFLMAO:
By rights women should make brilliant welders because they can multi-task :unsure:

I will try to go on a course at some point, my mate did this when he started & it is obviously the best way to start, but covid & the fact that when I'm working it is always away from home it doesn't make it that easy !!
In the meantime I'll practice in my garage & get help like all your advice when I'm struggling.

My machine is only DC so I won't be doing any alloy welding. I really only wanted/intended to weld bits to the bobber that I am building. After the first one I built it became a bit of a pain to take the bit & frame to my mate to get him or one of his welders to do the necessary. I thought it would be much better if I could at least tack the bracket or whatever in place & then just get him to final weld it for me. That way I didn't need to align/set-up/clamp everthing in place again while at my mates, before he could tack, then weld it in place.

Obviously as I get good at tacking things I'll want to get good at welding so like alot of things in life you are always striving to get better at something.
And don’t worry, we all started somewhere.. Your bad welds will teach you so much so don’t be ashamed of them, use them, get feedback and learn from them..

It’s like learning a Guitar etc, frustrating but if you practice WELL, you will get the results in time.. X
 
For those without a foot pedal these are standard settings for Mild and Stainless steel v the various joints..

I learnt without a pedal and although i have one i offer don’t use it tbh..

i would tend to set the Amps a little low to start and if you don’t get a nice fluid puddle that the angle of your torch/electrode can easily push along just increase it by 5 amps a time until you do..

A tight arc is the main issue when learning..

you need to be comfortable and have a free run for your torch to pass along its path without snags etc.. When you have this you need to get the arc ( tip of the electrode) down to 1-1.5mm from the puddle and be consistent with it..
Get your torch hand comfortable, if need be rest it on something to make it comfortable etc, this trust me makes such a difference..

Get a really good fit up if doing joints, really tight makes it so much easier.. The bigger the gap the harder it is...

If your struggling, try doing the above but without using filler rod.. Just run beads without filler on clean flat steel plate, then do the same and join two flat pieces together without filler rod, ( no gap between the two bits though) clamp the bits of steel down if you can also, stops it warping and moving around on your bench..

X


View attachment 7637

View attachment 7638
Maybe put a nice vid up so people can see how you do it?
 
Practice practice practice, Noods mentions starting with a lower amperage, this can be counter productive as a lower amperage means you are holding the torch on the material longer hence building up heat throughout the material before it's started to melt particularly with alloy, it's natural for beginners to use too low an amperage because we are frightened of blowing holes in the material and we cant run the bead fast enough but it doesn't always work that way. I never stop practicing and making fine adjustments and taking notes of my findings.
Steve
 
And don’t worry, we all started somewhere.. Your bad welds will teach you so much so don’t be ashamed of them, use them, get feedback and learn from them..

It’s like learning a Guitar etc, frustrating but if you practice WELL, you will get the results in time.. X
Balls...
I can't play the Guitar either... I was really hoping to get half good at welding, as I spent most of my life soldering and Brazing.
 